Northstar Polymers MSS-A80AQ High Performance Polyurethane Cast Elastomer System 80A
Manufacturer | Northstar Polymers |
Trade Name | |
Port | Ningbo port,China |
Trade Terms | FOB, CFR, CIF |
Payment Terms | L/C, T/T, Western Union |
Category Thermoset Polyurethane, Liquid
Description
Material Notes:
This is a Ester/MDI base high-performance polyurethane casting system. This systems is recommended to applications in which the part requires high tensile strength, cut/tear resistance, dry-abrasion resistance, slow response speed, and low energy rebound/response. Ester base systems are generally less expensive than PTMEG base material. Possible applications for this material include skirting for conveyer belts, abrasion resistance liners and parts, and other specialty parts. Unlike conventional full-prepolymer systems, quasi system formulation improves processability, in-mold flow, and components mixing by use of low viscosity prepolymer. This results better physical properties of the products. Can be approved for FDA dry food contact.Information provided by Northstar Polymers.
Mechanical Properties | Metric | English | Comments |
---|---|---|---|
Hardness, Shore A | 80 | 80 | ASTM D2240 |
Tensile Strength | 41.4 MPa | 6000 psi | ASTM D412 |
Elongation at Break | 900 % | 900 % | ASTM D412 |
Tear Strength | 61.4 kN/m | 350 pli | Split; ASTM D624 |
105 kN/m | 600 pli | Die C; ASTM D624 | |
Taber Abrasion, mg/1000 Cycles | 15 | 15 | ASTM D4060 |
Processing Properties | Metric | English | Comments |
---|---|---|---|
Processing Temperature | 21.1 °C | 70.0 °F | Prepolymer Temperature |
82.2 °C | 180 °F | Curing Agent Temperature | |
Mold Temperature | 82.2 °C | 180 °F | |
Cure Time | 30.0 min
@Temperature 82.2 °C
|
0.500 hour
@Temperature 180 °F
|
De-mold Time |
960 – 1440 min
@Temperature 82.2 °C
|
16.0 – 24.0 hour
@Temperature 180 °F
|
Complete Cure Cycle | |
Pot Life | 2.50 – 3.00 min | 2.50 – 3.00 min | |
Gel Time | 4.00 min | 4.00 min |
Descriptive Properties | Value | Comments |
---|---|---|
Curing Agent | SBA-036 | |
Prepolymer | MSA-018 | |
Weight Ratio | 1:1.978 | Prepolymer to Curing Agent Ratio |